Abstract
This paper focuses on some chemical and structural aspects for mature concrete structural substrate that functions as a barrier to radioactive material migration. Exposure to radioactive material may be a consequence of surface contact, such as exposure by spills or leaks. In properly-prepared waste storage area, undamaged paint and sealant helps to protect the structural cement. However, damaged surfaces, cracks, and relatively porous slab seams can offer a preferred migration pathway for spilled contaminates, including radionuclides.
The cost of remediation of concrete structures is directly related to the amount of concrete that must be removed and subsequently disposed. A carefully implemented investigative plan can be utilized to determine how much concrete must be removed and the approximate level of volumetric radiological contamination can be estimated to help bound disposal costs.
Normal concrete pore solution is saturated with calcium hydroxide and also contains sodium and potassium hydroxide; the pH is typically 13-14. Contaminants (such as uranium) that hydrolyze in alkaline media to form precipitant phases tend to deposit at the near-surface. However, more soluble contaminants, such as Cs-137 (as Cs+) and Tc-99 (as the pertechnetate anion, TcO4-) diffuse more deeply into the porous substrate. Profiling the migration of the water-soluble radionuclides into a cured (hardened) cement surface may be a challenge, since water-cooled saws, borers and similar implements are often used to excise and/or slice the core. Alternately, dry mechanical fracturing for excavation of cement may introduce the possibility of material cross-contamination and uncertainty for the average sampling depth for the sample collection event, potentially yield non-representative samples, and may preclude assessment of crack formation that may have been present in the native (nonfractured) substrate.
Structural concrete is comprised of cement and pozzolan paste, relatively impervious aggregate (typically stone and/or sand), and rebar (iron reinforcement). Near-surface aggregate may act as a hydrolytic barrier, causing contaminants leached into the porewater to by-pass the impervious grains, causing deeper-than-expected penetration, especially if there are grain boundary cracks also present to facilitate migration.
These effects are demonstrated for structural concrete slab cores, taken during Decontamination and Decommissioning activities at an NRC-licensed site, and also for small-scale test cylinders used to assess the rate of migration of uranium into the grout surface from contact with a caustic synthetic sludge. Polished epoxy-mounted cross-sections from the latter were subjected to limited petrology, including optical and electron microscopy. Elemental associations demonstrated that the penetration of uranium was generally limited to the first 100-150 microns of the exposed (“top”) surface, with preferential flow (“fingering”) around the silica aggregate. Samples of grout for a companion specimen from the same core were scraped from the “top” and “bottom” surfaces and the materials were characterized by X-ray diffraction (XRD), to facilitate the identity of potential new phases that may have formed. A tentative identification was made for a soddyite-type (uranyl silicate) phase, which is apparently formed as an alteration product as the poorly-soluble uranate-type phase in the wet sludge diffuses into the cement host.
The authors offer practical suggestions about obtaining a representative core sample of the concrete during sample preparation.